- Sapwood: greyish white to yellowish white.
- Heartwood: dark grey to reddish grey.
- Fiber: Straight, frequently intertwined.
- Grain: medium size
![Sucupira Sucupira](/sites/default/files/styles/large/public/2023-11/ef765f67211e4c219f57159ea0e792ae.jpg?itok=aXYzzJgj)
a
b
c
d
e
f
g
h
i
j
k
l
m
n
o
p
q
r
s
t
u
v
w
x
y
z
![Impregnabilidad](/themes/custom/gabarro/images/icons/impregnabilidad.png)
![Propiedades mecanicas](/themes/custom/gabarro/images/icons/propiedades-mecanicas.png)
![Mecanizacion logo](/themes/custom/gabarro/images/icons/mecanizacion.png)
![Propiedades fisicas logo](/themes/custom/gabarro/images/icons/propiedades-fisicas.png)
Impregnabilidad
- Sapwood: Medium capacity of being impregnated
- Heartwood: No capable of being impregnated
Propiedades mecánicas
- Resistance to static flexion 1,400 g/cm2
- Elasticity module 180,000 kg/cm2
- Resistance to compression 850 kg/cm2
Mecanización
- Sawing process: Common difficulties arise from hardness and abrasability
- Drying process: Medium to high speed. Low risk of deformation and crack formation.
- Planing process: Difficuties due to hardness, abrasability and risk of repelling on pieces of intertwined fibers. Slow mechanisation is recommended
- Gluing process: Tannins hamper proper adherence.
- Nailing and screwing process: pre-drilling is recommended due to hardness.
- Finish: No particular difficulties arise
Propiedades físicas
- Apparent density at 12% humidity 910 kg/m3 very heavy wood
- Dimensional stability
- - Volumetric contraction coefficient 0.44 % varies from stable wood to nervous wood
- - Relation between contractions 1.5% no tendency to deformity
- Hardness (Chaláis-Meudon) 8.3 very hard wood